Comparison

ABS Commodity vs PEEK

A side-by-side comparison of Acrylonitrile Butadiene Styrene Commodity Grades and Polyether Ether Ketone.

Physical

Density
1.04-1.08 g/cm³
1.32 g/cm³
Water Absorption (24h)
0.2-0.6 %
0.15 %
Transparency
Opaque
Opaque (amber)
Shrinkage
0.4-0.7 %
1.1 – 1.4 %

Mechanical

Young's Modulus
2.0-2.5 GPa
3.6 GPa
Tensile Strength
40-50 MPa
100 MPa
Elongation at Break
5-20 %
50 %
Impact Strength (Izod)
150-250 J/m
55 J/m
Flexural Strength
170 MPa

Thermal

Glass Transition Temperature
90-105 °C
143 °C
Melting Point
N/A (amorphous)
343 °C
Continuous Service Temperature
70-80 °C
260 °C
Heat Deflection Temperature
80-95 °C
160 °C

Electrical

Dielectric Constant
2.8-3.2
3.2
Volume Resistivity
10¹¹-10¹³ Ω⋅cm
10¹⁶ Ω·cm
Dielectric Strength
15-25 kV/mm

Chemical resistance

Acids
Good resistance
Excellent
Bases
Good resistance
Excellent
Solvents
Attacked by aromatic and chlorinated hydrocarbons, ketones, esters
Excellent
UV Resistance
Poor (requires stabilization)
Fair
Hydrolysis (steam)
Excellent

Sustainability

Recyclability
Recyclable
Recyclable (specialty)
Recycling Code
7 (Other)
7
Carbon Footprint
Moderate to High
~30 kg CO₂e / kg