Comparison
PPS GF40 vs PEEK
A side-by-side comparison of Polyphenylene Sulfide, 40% Glass Fiber Reinforced and Polyether Ether Ketone.
Physical
Density
1.60-1.70 g/cm³
1.32 g/cm³
Water Absorption (24h)
0.01-0.05 %
0.15 %
Transparency
Opaque
Opaque (amber)
Shrinkage
0.2-0.5 %
1.1 – 1.4 %
Mechanical
Young's Modulus
12-15 GPa
3.6 GPa
Tensile Strength
80-120 MPa
100 MPa
Elongation at Break
2-5 %
50 %
Impact Strength (Izod)
5-10 kJ/m
55 J/m
Flexural Strength
—
170 MPa
Thermal
Glass Transition Temperature
100-120 °C
143 °C
Melting Point
275-285 °C
343 °C
Continuous Service Temperature
200-240 °C
260 °C
Heat Deflection Temperature
250-270 °C (1.8 MPa)
160 °C
Electrical
Dielectric Constant
3.0-3.5
3.2
Volume Resistivity
10^12-10^14 Ohm-cm
10¹⁶ Ω·cm
Dielectric Strength
15-20 kV/mm
—
Chemical resistance
Acids
Excellent
Excellent
Bases
Excellent
Excellent
Solvents
Excellent
Excellent
UV Resistance
Good
Fair
Hydrolysis (steam)
—
Excellent
Sustainability
Recyclability
Recyclable (difficult processing)
Recyclable (specialty)
Recycling Code
7 (Other)
7
Carbon Footprint
High
~30 kg CO₂e / kg